A LiInSe2 neutron detector offers a way to absorb thermal neutrons and collect the resulting charge in one semiconductor, rather than relying on a separate neutron-converter coating. But detector performance depends on more than the material’s neutron-capture potential: deviations from the ideal crystal composition can create defects that trap charge carriers. Results from stoichiometry-focused crystal growth show how composition control can improve charge transport and alpha-particle response.

Why consider a homogeneous semiconductor neutron detector?

Conventional thermal-neutron detection approaches include scintillators and semiconductor sensors paired with neutron-active converter materials. In coated designs, increasing converter thickness can raise neutron absorption, but charged particles produced by neutron capture may be trapped in the converter before reaching the charge-collecting semiconductor. This creates a trade-off between absorption and charge collection.

LiInSe2 is a different approach: lithium in the crystal can capture a neutron, and the resulting reaction products generate charge carriers within the same material that collects them. The isotope 6Li has a large thermal-neutron capture cross-section; the cited work notes that a 3.4 mm-thick wafer containing 6Li can absorb more than 95% of incident neutrons. The practical challenge is preserving sufficient crystal quality for those generated carriers to be collected effectively.

How LiInSe2 stoichiometry affects detector performance

LiInSe2 crystals grown from a melt can deviate from the intended 1:1:2 ratio of lithium, indium and selenium. Loss of lithium and selenium during processing can contribute to vacancies and other native defects. Reported defects include lithium and indium vacancies or interstitials, selenium vacancies, and antisite defects in which lithium and indium occupy each other’s lattice sites.

These defects matter because they can act as carrier trapping or scattering centers. Reduced carrier transport limits charge collection efficiency, which can broaden a detector’s measured energy response. The reported spread in band gap and crystal color—from red to yellow—also reflects differences in the material. First-principles calculations identify indium-on-lithium and lithium-on-indium antisite defects as important contributors to the color variation.

Low-temperature synthesis supports composition control

To reduce component loss, the researchers used a relatively slow, lower-temperature synthesis process for polycrystalline LiInSe2 before growing single crystals by the vertical Bridgman method. The controlled heating from 180°C to 250°C was intended to encourage the formation of intermediate lithium-selenium and indium-selenium compounds while limiting lithium activity and selenium evaporation. The material was then heated further to form the target compound.

Inductively coupled plasma measurements showed that the resulting crystals were closer to the intended stoichiometric composition than several previously reported examples, although some samples remained cation-rich. The work therefore demonstrates a route toward composition control, not a guarantee that every grown crystal will be perfectly stoichiometric. Crucible materials and the amount of excess lithium and selenium used during synthesis also formed part of the growth conditions.

Electrical and optical properties of the crystals

The grown crystals had room-temperature resistivities in the range of approximately 1011 to 1012 Ω·cm. High resistivity is valuable in a radiation detector because it is associated with low dark current, helping limit background electrical current during measurement. The yellow crystal’s measured resistivity was 6.1 × 1011 Ω·cm; red and light-red samples measured 1.7 × 1012 and 8.1 × 1011 Ω·cm, respectively.

Measured optical band gaps varied with crystal color, from 2.01 eV for the dark-red sample to 2.83 eV for the yellow sample. The calculations predicted a lower direct band gap of 1.612 eV, which the authors attribute to the known tendency of the calculation method to underestimate band gaps. The distinction between calculated and measured values is important when interpreting material models alongside experimental detector data.

Charge collection and alpha-particle response

Detector response was evaluated using 5.48 MeV alpha particles from an 241Am source. The alpha-particle energy resolution varied across the three wafers: 43.1% for the dark-red crystal, 28.9% for the light-red crystal and 23.3% for the yellow crystal. The yellow sample also had the highest reported electron mobility-lifetime product, approximately 2.5 × 10-5 cm2V-1, compared with 1.5 × 10-5 and 9.3 × 10-6 cm2V-1 for the other wafers.

The relationship between composition and response is consistent with fewer performance-limiting defects in crystals closer to the intended composition. In particular, antisite defects associated with the red samples can interfere with carrier transport. These measurements use alpha particles as a way to characterize charge collection; they are not, by themselves, a complete demonstration of operational neutron-detector performance.

Implications for neutron-detector development

The study also reported a dull response to 1.33 MeV gamma radiation from a 60Co source under the tested conditions, alongside a clear alpha-particle response. This observation suggests potential for neutron/gamma discrimination, but it should be understood within the limits of the reported measurement rather than treated as a universal performance guarantee.

For engineers and materials developers, the central lesson is that detector-grade LiInSe2 depends on controlling composition through synthesis and crystal growth. Resistivity, band gap, native defects and charge collection are interrelated indicators of material quality. The yellow crystal’s 23.3% alpha-particle energy resolution and higher mobility-lifetime product illustrate the performance associated with improved charge transport in the samples studied.

Further progress will require continued refinement of melt-growth procedures and defect control. For system designers evaluating semiconductor neutron detection, LiInSe2 is a promising material, while reproducible stoichiometry and effective charge collection remain key considerations in translating crystal properties into detector performance.