Access Official Technical PDF

Share Summary:LinkedInEmail

Mid-infrared optical fiber development depends on more than the choice of an active ion. The glass must transmit in the target wavelength range, limit mechanisms that quench emission and remain stable enough to form into a fiber. A study of holmium- and ytterbium-co-doped bismuth-germanate glass examined these requirements together, producing a fiber core that emitted near 2.87 µm under 980 nm excitation.

The work is relevant to engineers and technical decision-makers assessing optical sources for applications such as atmospheric pollution monitoring, remote sensing and other mid-infrared systems. Its practical contribution is a material design that combines a low maximum phonon energy with reduced hydroxide content, effective energy transfer between dopants and sufficient thermal stability for fiber processing.

Why bismuth-germanate glass for mid-infrared optical fiber?

Glass composition influences both the wavelengths a material can transmit and how efficiently rare-earth ions can emit. Many conventional oxide glasses have phonon energies that limit mid-infrared transmission or emission. Some non-oxide glasses offer lower phonon energy, but their thermal stability can make processing into photonic structures more challenging.

Bismuth-based heavy metal oxide glasses offer a potential balance. The investigated bismuth-germanate host had a measured maximum phonon energy of 724 cm-1, a reported transmission window from approximately 0.51 to 5.5 µm, and a thermal stability parameter of 124 °C. That parameter is the difference between the crystallization temperature, 532 °C, and the glass transition temperature, 408 °C. The reported melting temperature was 773 °C.

These properties matter together: a material intended for an active fiber must support the optical behavior of its dopants while tolerating the steps required to form a fiber. The study’s thermal results indicated that this glass could be considered for fiber drawing; they do not, by themselves, establish performance in a complete laser or amplifier system.

Reducing hydroxide absorption near 3 µm

A significant design challenge for glass operating near 3 µm is absorption associated with hydroxide ions. In this material, that absorption appears around 3.1 µm and can reduce transmission in a region important to mid-infrared applications. Hydroxide-related losses can also act against useful fluorescence.

To reduce hydroxide content, the glass was synthesized under low-vacuum conditions of 45–65 mBar. Measurements estimated a hydroxide concentration of 47 ppm and an absorption coefficient of 0.11 cm-1 at the absorption feature. These results support the value of controlling the glass-making environment when developing an optical material for operation near this wavelength range.

The measurements also illustrate why evaluating only an emission peak is insufficient. Transmission, absorption and the glass structure all influence whether a material can serve as a useful active fiber core.

How ytterbium sensitizes holmium emission

Holmium ions produce the emission of interest through the 5I6 to 5I7 transition, centered at 2.87 µm in the reported measurements. However, direct excitation of Ho3+ at 980 nm is not effective because its ground-state absorption does not overlap suitably with that pump wavelength.

Ytterbium provides a route to excite the holmium ions. Yb3+ absorbs near 980 nm and can transfer energy to Ho3+, populating the holmium level responsible for the 2.87 µm emission. In this arrangement, ytterbium acts as a sensitizer and holmium as the emitter.

The researchers compared dopant concentrations and found the strongest 2.87 µm emission among the tested compositions in glass containing 0.25 mol% Ho2O3 and 0.75 mol% Yb2O3. Increasing ytterbium content while holding holmium at 0.25 mol% enhanced the emission across the tested samples. Reducing holmium concentration at a fixed ytterbium content of 0.75 mol% reduced the mid-infrared emission.

Lifetime measurements provided evidence for the energy-transfer process. The measured lifetime of the Yb3+ excited state was 266 µs in the co-doped glass, compared with 684 µs in the ytterbium-only glass. From these values, the energy-transfer efficiency was calculated as 61%.

From glass sample to active fiber core

The composition with the strongest measured emission was used as the core of an optical fiber, with silicate glass as the cladding. The reported fiber had a 120 µm core diameter and a 250 µm cladding diameter. The core refractive index was 2.19, and the numerical aperture was close to 1.

Under 980 nm pump radiation, the fiber produced a band centered near 2.87 µm. Compared with the bulk glass, its emission band narrowed from a full width at half maximum of 80 nm to 71 nm, with a 6 nm shift toward longer wavelengths. The study attributed these changes to reabsorption of the generated signal as it traveled along the fiber core.

Practical implications for photonic system development

For engineers evaluating mid-infrared sources, this work highlights several material-level considerations:

  • Control hydroxide content: synthesis conditions can affect absorption near 3 µm, so process control is relevant to the optical design.
  • Match sensitizer and emitter concentrations: the measured emission depended on the Ho3+/Yb3+ composition, with 0.25/0.75 mol% identified as optimal among the tested samples.
  • Assess the host glass as a whole: phonon energy, transmission range and thermal stability influence both emission potential and fiber fabrication.
  • Account for propagation effects: the fiber spectrum differed from the bulk-glass spectrum, consistent with reabsorption along the core.

The results establish a material and fiber demonstration, not a complete application-ready laser or amplifier specification. System-level design would need to consider the requirements of the intended source, including its pumping and optical configuration.

Conclusion

Ho3+/Yb3+-doped bismuth-germanate glass combines low phonon energy, a broad reported transmission window and reduced hydroxide absorption with measurable energy transfer under 980 nm excitation. Its conversion into an active fiber that emits near 2.87 µm demonstrates a potential route toward mid-infrared optical sources. For photonics developers, the key takeaway is to treat glass composition, hydroxide control, dopant balance and signal propagation as connected design variables when evaluating fiber-based mid-infrared systems.

Access Official Technical PDF

About The Author