Developing a practical CdTe back contact means balancing electrical performance with the optical transparency needed for bifacial or tandem solar-cell designs. A CuS-ZnS nanocomposite thin film offers one possible route: it can act as a p-type hole transport layer at the rear of the absorber while allowing visible light to pass. Device tests show improved performance in some contact configurations, but also illustrate why transparency alone is not enough to make a bifacial CdTe cell effective.
Why transparent back contacts matter
In a conventional CdTe solar cell, the rear contact must collect holes from the absorber without creating excessive resistance or recombination. This is challenging because CdTe’s deep valence band can contribute to a barrier at the rear interface. A transparent back contact adds another requirement: light entering through the rear must reach the absorber, which is important for bifacial devices and can also support tandem-cell concepts.
The study evaluates a nanocomposite made from copper sulfide and zinc sulfide, written as (CuS)x(ZnS)1-x. The material is p-type and is used as an interface layer between CdTe and a metal contact or transparent indium tin oxide (ITO) electrode. The intended role is to support hole transport while reducing losses associated with the CdTe rear interface.
CuS-ZnS nanocomposite properties and deposition
The films were deposited using chemical bath deposition, a solution-based process in which a substrate is immersed in a precursor solution. The reported approach produced thin, compact films at a bath temperature of 80 °C. At approximately 45 nm thick, the films transmitted more than 70% of visible light. For the tested composition, (CuS)0.64(ZnS)0.36, microscopy showed compact grains approximately 10 nm in size.
Optical and electrical characterization indicated that the material combines visible-light transparency with high carrier concentration. The researchers reported a carrier density on the order of 1021 cm−3 and a band gap of approximately 2.7 eV for the 0.64 composition. These properties support its proposed use as a hole transport layer rather than as the primary light-absorbing layer of the solar cell.
CdTe back contact results with metal electrodes
In opaque devices using a conventional Cu/Au metallization process, inserting the nanocomposite between CdTe and the contact produced a best reported efficiency above 13%. The study describes this peak result as a 3.2% relative improvement over the standard Cu/Au back contact. In the averages across 20 cells, the (CuS)0.64(ZnS)0.36/Cu/Au configuration reached 12.6% efficiency, compared with 12.1% for Cu/Au alone.
The comparison also showed differences between compositions. The average efficiency for the 0.80 CuS-fraction composition was 11.8%. The 0.64 composition had the higher average short-circuit current density among the nanocomposite variants tested. External quantum efficiency measurements showed slightly improved current collection across part of the 550–820 nm range when the nanocomposite was used.
A separate comparison omitted the copper evaporation and annealing steps, using the nanocomposite with gold instead. In that test, the average efficiency was 10.5%, versus 7.5% for gold alone. The nanocomposite/Au devices also showed higher average open-circuit voltage and fill factor. These results indicate that the interface layer can matter independently of the added copper process, although outcomes depend on the complete contact stack.
Why back illumination remains difficult
To assess bifacial operation, the researchers added ITO as a transparent rear electrode. The device performed substantially better under front illumination than under rear illumination. For the ITO-finished devices, the reported average efficiency was 9.2% from the front and 1.4% from the back. The authors also reported a best front-illuminated device efficiency of 10.5%, underscoring that results vary by whether peak or average device performance is being discussed.
The main limitation is carrier collection through the CdTe absorber. Under back illumination, many photons generate carriers away from the junction’s charge-separating electric field. Electrons generated near the rear must travel through the absorber toward the front junction, where they can recombine before collection. The study’s modeling and measurements associate the losses with the absence of a charge-separating field near the back contact, interface recombination, and insufficient electron diffusion length.
ITO and the nanocomposite can provide a transparent rear-side contact structure, but they do not by themselves create the internal field needed to collect carriers efficiently when light enters from that side. The tested devices also had higher series resistance with the transparent contact stack, which affected fill factor. Improving the interface and increasing carrier lifetimes in the CdTe absorber are therefore important considerations for further development.
Practical implications for solar-cell development
For photovoltaic engineers and device developers, the results distinguish two related but separate tasks:
- Improve rear-interface transport: The nanocomposite layer showed potential to improve performance when used with metal back contacts.
- Enable useful rear illumination: Bifacial operation also requires effective carrier separation and collection across the absorber, not simply a transparent electrode.
- Manage contact resistance and recombination: The full layer stack, including the interface and transparent electrode, influences device behavior.
- Optimize the absorber and interface together: The modeling points to interface quality and CdTe carrier lifetime as important factors for reducing back-illumination losses.
The CuS-ZnS nanocomposite is a promising candidate for a transparent, earth-abundant CdTe interface layer, with chemical bath deposition providing a solution-based fabrication route. Its demonstrated performance gains with metal contacts are encouraging, but the bifacial results show that transparency is only one part of the design problem. For practical bifacial CdTe cells, contact engineering must be paired with improved charge separation and carrier collection so that light entering from either side can contribute effectively.