Grain-dependent corrosion can make the electrochemical response of a steel surface vary over very short distances. For engineers assessing materials in acidic environments, that variation matters: grains with different crystal orientations may not dissolve at the same rate, even when they are part of one continuous steel component. A study of low-carbon steel shows how nanoscale electrochemical measurements, combined with structural characterization, can reveal this relationship in detail.
Why steel microstructure matters to corrosion
Steel microstructure includes grains with different crystallographic orientations, as well as grain boundaries and inclusions. These features can influence the local anodic and cathodic reactions involved in corrosion. Yet establishing a reliable link between a specific surface feature and its electrochemical behavior is challenging. Measurements made at only a few locations may miss important variation or produce too little data to compare grain orientations confidently.
The challenge is particularly relevant when examining metal dissolution. Conventional scanning electrochemical microscopy can detect local activity indirectly by measuring electrochemical species or fluxes near a surface. Interpreting results at a corroding interface can be complicated by changing topography and by the range of products and intermediate species present. Electrochemical droplet cells instead contact a small area and measure its response directly, but conventional versions have limited spatial resolution and throughput.
Mapping grain-dependent corrosion with SECCM
Scanning electrochemical cell microscopy (SECCM) extends the droplet-cell approach. A fine nanopipet forms a small electrolyte meniscus on the material, creating a local electrochemical cell. The probe can move between locations and make measurements across a surface, enabling spatially resolved mapping rather than relying on a handful of larger-area tests.
In the study, a nanopipet containing dilute sulfuric acid contacted a polished low-carbon steel surface. At each location, researchers recorded a potentiodynamic polarization response: the applied potential was swept while the resulting current was measured. The surface was then characterized with electron backscatter diffraction (EBSD), which identifies the crystallographic orientation of grains. This made it possible to compare local electrochemical measurements with the structure at corresponding positions.
The measurements focused on low-index planes in the body-centred cubic steel structure: (100), (101) and (111). Hundreds of individual measurements were collected across these orientations. This level of sampling is important because it allows differences between groups of grains to be distinguished from point-to-point variation.
Orientation changes the rate of iron dissolution
Under the tested conditions—aqueous sulfuric acid at pH 2.3—the rate of anodic iron dissolution varied with crystal orientation. The measured dissolution rate increased in the order (101) < (111) < (100). In other words, the (100) orientation showed the greatest dissolution response among the three planes examined, while the (101) orientation showed the least.
The polarization measurements also distinguished different stages of the electrochemical response. At more positive potentials, the steel surface was in a passive state, associated with a protective oxide film. As the potential changed, a reduction feature indicated removal of that film. In the active region, iron dissolution produced a pronounced anodic current. The study found that the onset of active dissolution and the magnitude of the current varied among grains.
These results apply to the specific material and acidic test conditions used; they should not be treated as a universal ranking for all steel grades, electrolytes or service environments. The authors note that corrosion behavior can depend on solution conditions. The observations nevertheless demonstrate why surface structure needs to be considered when interpreting local corrosion measurements.
Combining electrochemistry with structural and computational analysis
SECCM provided local electrochemical data, while EBSD linked that response to grain orientation. Additional scanning transmission electron microscopy (STEM) examined cross-sections through individual measurement sites. The images showed a recess associated with iron removal and corrosion products deposited over the affected area. Elemental analysis detected iron, sulfur and oxygen in the deposit; iron oxysulfate species were proposed as likely products based on thermodynamic calculations.
Density functional theory (DFT) calculations offered a further way to examine the orientation trend. The calculations estimated the energy required to remove and ionize iron atoms at the surfaces of the different crystal planes. The experimental dissolution rates correlated with these calculated energies: orientations where surface iron was calculated to be easier to remove had higher measured dissolution rates.
This relationship provides a possible explanation for the observed differences, rather than a complete description of corrosion in every environment. The calculations represent a simplified system and do not explicitly account for all solution species. Their value here is in complementing the measurements with an atomic-scale perspective.
Practical implications for materials assessment
For engineers and materials teams, the main lesson is methodological: average corrosion measurements can conceal meaningful local variation. A surface may appear to have one overall electrochemical response while individual grains differ in their susceptibility to anodic dissolution. Local mapping can help identify and compare these differences, especially when measurements are correlated with structural data from the same area.
The study also illustrates the value of combining complementary methods:
- SECCM maps local electrochemical activity across a surface.
- EBSD identifies the crystallographic orientation associated with each measured region.
- STEM examines physical changes and corrosion products at selected sites.
- DFT helps assess whether calculated atomic-scale energetics align with measured trends.
Together, these techniques offer a more detailed way to investigate how microstructure relates to corrosion behavior than electrochemical measurements alone. For practical assessment, results should be interpreted in the context of the material, electrolyte and test conditions rather than generalized beyond them.
Conclusion
Nanoscale mapping revealed that low-carbon steel grains with different crystallographic orientations can exhibit different rates of anodic iron dissolution in acidic sulfuric acid. In the conditions tested, dissolution increased from (101) to (111) to (100). Pairing SECCM measurements with EBSD, microscopy and DFT helped connect local electrochemical behavior to both grain structure and calculated surface energetics. The practical implication is clear: resolving corrosion at the scale of microstructure can provide information that bulk or sparse measurements may not capture.