Access Official Technical PDF

Share Summary:LinkedInEmail

Vertical GaN power devices depend on carefully engineered drift layers: these regions must support high voltage while maintaining the electrical properties needed for power conversion. Hydride vapor phase epitaxy (HVPE), traditionally associated with fast growth of thick GaN, is being explored as an alternative way to produce the very lightly doped material these devices require. Work by SCIOCS and Hosei University illustrates both the promise of HVPE and the process tradeoffs involved in combining it with other epitaxial methods.

Why the GaN drift layer matters

In a vertical power device, the drift layer provides the distance over which voltage drops. A suitably designed layer helps reduce the electric field within the material and supports a higher breakdown voltage. Its doping and uniformity therefore affect how consistently a device behaves across its active area.

GaN is of interest for power conversion because of its high critical electric field and high-frequency capability. But realizing those material advantages in a device requires control of impurities and carrier concentration, as well as a high-quality layer structure. The reported work examines whether HVPE can contribute to that control, rather than being used only to grow thick bulk material.

HVPE for vertical GaN power devices

SCIOCS and Hosei University compared a hybrid epitaxial structure with one produced entirely by metal-organic chemical vapor deposition (MOCVD). In the hybrid approach, HVPE formed the n-type GaN drift layer, followed by MOCVD regrowth. The comparison MOCVD-only process required a more complex n-type drift-layer structure. Before regrowth, the HVPE-grown material was cleaned using a hydrofluoric-acid process.

The researchers used an HVPE chamber designed without quartz components in its high-temperature areas. This addresses a specific materials concern: silicon and oxygen can act as donor impurities in GaN, and quartz is a potential source of both. MOCVD also uses metal-organic precursors, which can contribute carbon incorporation. In the reported work, secondary-ion mass spectrometry (SIMS) found no detectable carbon in the HVPE drift layer.

Earlier work by the team found that removing quartz from high-temperature chamber areas reduced oxygen and carbon below the measurement system’s detection limit. Process optimization also brought silicon below the stated SIMS detection limit of 5 × 1014 cm-3. These findings help explain why quartz-free HVPE was considered for the diode study: it offered a way to limit unintended impurities associated with the growth environment.

Impurity control and device uniformity

Impurity levels matter not only for the average electrical properties of a wafer, but also for their consistency across it. The researchers reported that the quartz-free HVPE drift layer reduced conductivity non-uniformity associated with carbon incorporation and uncontrolled silicon. Electroluminescence observations were used to identify variations in device behavior.

In the MOCVD material discussed in the study, carbon incorporation and compensation effects varied in connection with surface macrosteps tens of microns in scale. By contrast, SIMS confirmed the absence of carbon in the HVPE drift layer. The team argued that reducing carbon compensation and in-plane carrier-concentration modulation could make it easier to grow device structures closer to their intended design. They also highlighted the potential relevance of more uniform performance when wafer off-angle varies, including as a result of wafer bowing.

These results point to a process opportunity, not a guarantee of production performance. For device developers and integrators, the practical question is whether the reduced impurity-related variation can be maintained alongside reliable interfaces, repeatable epitaxy, and the desired device characteristics.

What the hybrid diode results show

The vertical pn diode was fabricated with mesa etching for isolation and palladium/titanium/gold and indium tin oxide contacts for the p- and n-sides, respectively. A 200-micron-diameter hybrid diode reached a reported breakdown voltage of about 2 kV and an on-resistance of 2 mΩ·cm2. It did not use a field plate, which the researchers omitted to avoid field concentration at electrode edges.

The device also showed low-forward-bias leakage, and its ideality was around 2, compared with approximately 1 for the MOCVD-only comparison structure. The researchers suggested that recombination through defects or impurity levels, potentially associated with silicon accumulated at the regrowth interface, could explain the deterioration. Despite that limitation, they reported that the hybrid diode’s observed characteristics were superior to those of a previously reported similar diode with an MOCVD-grown drift layer and an MBE-regrown p-GaN layer.

For engineering teams, this is an important distinction: drift-layer quality is only one part of the device stack. Regrowth interfaces and defect-related current can influence diode behavior, so process choices must be assessed across the complete structure rather than by considering impurity reduction alone.

Thick GaN substrates and manufacturing considerations

SCIOCS also developed free-standing GaN using a void-assisted separation method. A thin MOCVD GaN seed layer containing nanoscale voids is first formed on sapphire. HVPE GaN then nucleates as islands, coalesces, and grows thicker. The wafer initially bows and later becomes less bowed as growth proceeds. The method was used to produce substrates ranging from 100 microns to more than 6 millimeters thick.

Thick growth creates a stress-management challenge. Bowing changes and impurity incorporation near the wafer edge can contribute to stress and cracking. The researchers reported that controlling HVPE growth conditions to increase crystal hardness helped reduce the risk of cracking while lowering threading dislocation density. Their reported work included a 6-millimeter-thick, 55-millimeter-diameter substrate without macro-defects and with threading dislocation density in the mid-105 cm-2 range. They also reported 4-inch and 6-inch free-standing wafers thicker than 3 millimeters; the 6-inch material was described as being processed and not yet characterized in the account.

Practical implications for device development

HVPE offers a potential route to low-doped GaN drift layers, while quartz-free chamber design can help limit unwanted impurity incorporation. The hybrid diode results demonstrate that the approach can support high-voltage operation, but also underline the importance of regrowth interfaces and defect-related leakage. In parallel, thick free-standing substrates address a different part of the materials challenge: producing GaN crystals suitable for device platforms while managing stress and defects.

For industrial automation and power-electronics teams evaluating vertical GaN, the key takeaway is to assess the entire materials and device process. Growth method, impurity control, wafer uniformity, substrate quality, and interface behavior all influence whether the theoretical advantages of GaN translate into repeatable device performance.

Access Official Technical PDF

About The Author