As renewable generation, energy storage and electric vehicles expand, power conversion systems must handle electricity efficiently across a wider range of applications. Silicon carbide (SiC) power devices are increasingly used to reduce conversion losses. For manufacturers, however, device performance depends not only on the semiconductor material but also on the quality of the SiC epitaxial wafer on which devices are built.
The epitaxial layer forms the drift region in a power device. Its thickness and doping concentration influence important electrical characteristics, including blocking voltage and on-state behavior. As SiC substrates grow to 6 inches and device dies become larger, controlling defects and maintaining uniform epitaxial growth across the wafer are essential manufacturing challenges.
Why SiC epitaxial wafer quality matters
SiC power devices are fabricated on an epitaxial layer grown over a SiC substrate. Variations in layer thickness or doping concentration can contribute to differences in device characteristics across a wafer. Defects can also reduce performance or reliability, making their density and distribution important considerations for production yield, particularly as die sizes increase.
SiC epitaxy is commonly performed by chemical vapor deposition (CVD) at temperatures of approximately 1,500°C or higher. The process must manage heat and gas reactions consistently across the wafer surface. These demands become more complex when a reactor processes multiple large wafers, because temperature variation can affect growth conditions and the resulting layer.
Surface defects such as down-falls and triangular defects are examples of potential device-killer defects. Down-falls can result when particles or byproducts land on the growing surface. Triangular defects can contain stacking faults. Both defect types need to be controlled because they can adversely affect devices formed in the epitaxial layer.
Managing dislocations during SiC epitaxial growth
SiC substrates produced by sublimation growth can contain several types of dislocations, including threading edge dislocations, threading screw dislocations and basal plane dislocations (BPDs). A BPD that propagates from the substrate into the epitaxial layer can contribute to stacking-fault expansion when a device carries bipolar current. This mechanism can degrade device reliability.
One approach is to encourage BPDs to convert into threading edge dislocations (TEDs) during epitaxial growth. TEDs are generally considered less harmful in this context. Conversion is not automatic: the proportion of BPDs that continue into the epitaxial layer depends on growth conditions.
In the reported 6-inch wafer development, introducing a buffer layer during the early growth stage helped promote BPD conversion. The BPD density in the epitaxial layer was reduced to 0.1 cm-2 or less. In a defect-free-area assessment using 2.6 × 2.6 mm2 photoluminescence imaging fields, 99.9% of the measured area sections contained no BPDs.
Hot-wall CVD and temperature control
The process used a hot-wall CVD reactor designed to grow epitaxial layers on multiple 6-inch wafers at once. Wafers are placed on a rotating graphite susceptor inside a quartz chamber. An induction heater supplies heat, while thermal insulation surrounds the susceptor. Silane and propane serve as precursor gases, hydrogen acts as the carrier gas, and the process operates at low pressure.
Thermofluid simulation showed why temperature management matters. Without susceptor rotation, the upstream region exposed to incoming gas was cooler, in part because the hydrogen carrier gas removed heat. Rotation reduced temperature differences across the susceptor, but a cooler tendency remained at its outer edge. The center was also cooler, possibly because heat was carried away through the rotating rod.
These patterns can affect growth behavior across the wafer. The outer region, in particular, can experience temperature changes that influence gas reactions and doping concentration. Simulation-informed process development can therefore help address nonuniform conditions rather than treating the wafer surface as thermally uniform.
Reducing killer defects and stabilizing production
Defect reduction also requires attention to the reactor environment and the start of epitaxial growth. Cleaning the reactor interior helps limit foreign particles that could fall onto the wafer. Stabilizing and optimizing surface growth when precursor gases are introduced can help reduce defects associated with early growth stages.
After process improvements, the reported average densities were 0.05 cm-2 for down-fall defects and 0.08 cm-2 for triangular defects. Across 20 epitaxial layers grown on 6-inch wafers, the average density of each assessed defect type was below 0.1 cm-2; the average BPD density was 0.1 cm-2. These results indicate the importance of evaluating both the achieved defect levels and their repeatability across multiple growth runs.
Defect distribution must also be considered in relation to die area. In the evaluated epitaxial material, approximately 99% of 2 × 2 mm2 areas were defect-free. For a 5 × 5 mm2 area, the reported defect-free proportion was approximately 98%. Larger device areas are more likely to intersect a defect, so wafer-level maps can help manufacturers assess the implications for different die designs.
Uniformity supports consistent device characteristics
In a 6-inch wafer demonstration targeting a 10 μm epitaxial layer and a doping concentration of 8 × 1015 cm-3, thickness measurements across 41 points averaged 10.1 μm, ranging from 9.9 to 10.6 μm. The standard deviation relative to the average was 1.9%. Doping concentration averaged 8.1 × 1015 cm-3, with measurements from 7.6 × 1015 to 8.4 × 1015 cm-3 and a standard deviation-to-average ratio of 2.2%.
For process and device teams, these measurements illustrate the need to assess more than a wafer’s average values. Spatial uniformity in thickness and doping matters because both can influence device-characteristic variation across the wafer.
Practical implications for SiC device manufacturing
Producing high-quality SiC epitaxy on larger wafers calls for coordinated control of substrate dislocations, reactor cleanliness, early-stage growth, temperature distribution and layer uniformity. The reported results show that buffer-layer growth and process optimization can reduce defects while maintaining controlled thickness and doping across multiple 6-inch wafers. For manufacturers, the practical objective is consistent epitaxial material that supports predictable device characteristics, larger die designs and the reliability requirements of high-current power applications.