In silicon solar cells and photoelectrochemical (PEC) devices, the interface between the silicon absorber and its electrical contact has to perform two jobs: limit charge-carrier recombination and allow the desired carriers to flow. Research on tantalum oxide silicon solar cells demonstrates how an ultrathin TaOx layer can help meet both requirements, with potential relevance to interface engineering across optoelectronic devices.
The reported devices used an approximately 6 nm TaOx film as an electron-selective heterocontact. The layer was evaluated in crystalline silicon (c-Si) photovoltaic cells and in photocathodes for water reduction. The results show why material selection, surface treatment, and thickness control must be considered together when developing functional thin-film interfaces.
Why an electron-selective contact matters
Silicon devices generate electrons and holes when they absorb light. To produce useful electrical output or drive a chemical reaction, the two carrier types must be directed toward separate terminals. Conventional approaches use doped regions in or on the silicon. A metal-insulator-semiconductor (MIS) heterocontact offers another route: a thin interlayer passivates the silicon surface while helping favor transport of one carrier type.
For an electron-selective contact, electrons should pass from silicon toward the outer contact, while holes should be blocked from following the same path. At the same time, defects at the silicon surface must be passivated. If recombination remains high, carriers can be lost before collection; if the interlayer impedes electron transport, contact resistance can compromise device operation. PEC applications add another requirement: the contact materials must withstand the chemical environment during operation.
Ultrathin silicon dioxide is a well-studied option, but its insulating nature can make transport dependent on tunnelling or pinholes. Its performance also requires tight control of a very small film thickness. TaOx was investigated as an alternative because its band alignment can support electron transport while its large valence-band offset presents a barrier to holes. The material also showed useful chemical stability for the aqueous PEC application.
TaOx interface treatment changes contact behavior
The TaOx films were deposited using atomic layer deposition (ALD). As deposited, the approximately 6 nm layer provided poor silicon surface passivation: the effective minority-carrier lifetime was about 30 microseconds at an excess carrier density of 1015 cm-3. After treatment using a plasma-enhanced chemical vapor deposited silicon nitride (SiNx) cap, the lifetime increased to approximately 650 microseconds at the same carrier density.
The SiNx cap was subsequently removed. The improvement was attributed mainly to hydrogen supplied during the capping process, which passivated defects at the TaOx/silicon interface. Measurements also showed a change in the oxide following hydrogenation: its oxygen-to-tantalum atomic fraction decreased slightly, and its measured work function was about 0.3 eV lower than that of the as-deposited film.
Electrical contact measurements showed a similarly important effect of the treatment. Before hydrogenation, the contact had strongly rectifying behavior. After hydrogenation, the approximately 6 nm TaOx contact to n-type silicon showed Ohmic behavior, with a reported contact resistivity of about 0.35 Ω·cm2. Together, the lifetime and contact measurements indicate that passivation alone is not enough; the interface must also permit adequate carrier transport.
Thickness control defines the performance trade-off
TaOx thickness affected both surface passivation and contact resistance. As film thickness increased, effective carrier lifetime initially improved and then approached a plateau, with the highest reported lifetime around 2.7 milliseconds at a thickness of 8 nm. Contact resistivity, however, rose as the layer became thicker and increased sharply beyond approximately 6 nm. At thicknesses above 10 nm, the contact again behaved in a rectifying manner after treatment.
This trade-off appeared in the completed photovoltaic devices. Efficiency increased as improved passivation supported higher open-circuit voltage and current, but declined at greater thicknesses as contact resistance affected the fill factor. The best-performing proof-of-concept cell used an approximately 6 nm TaOx layer and reached 19.1% conversion efficiency, compared with 17.1% for the control without TaOx. The TaOx cell also showed improved long-wavelength external quantum efficiency, consistent with reduced recombination at the rear silicon surface.
For process development, the finding is a reminder that a nominal material choice cannot be separated from the deposition and interface-treatment window. Film thickness, hydrogenation, and the metal contact all influence whether an interlayer functions selectively without creating an excessive transport barrier.
Applying the contact to photoelectrochemical water reduction
The researchers also tested TaOx in a silicon photocathode. For this configuration, the Mg/Ag contact used in the photovoltaic device was replaced with a Ti/Pt stack, with platinum serving as the catalyst surface for hydrogen evolution. The photocathode with TaOx reached a more positive onset potential and a higher photocurrent density than the control without the interlayer. Its applied-bias photon-to-current efficiency was 7.7%, an absolute improvement of 3.8 percentage points over the control.
The PEC efficiency remained below the photovoltaic result. The reported explanation included lower photovoltage and fill factor, as well as less favorable electron-contact energy alignment in the Ti/TaOx/silicon configuration than in the Mg/TaOx/silicon photovoltaic contact. This distinction highlights a practical design consideration: an interface that works in one device architecture may need re-optimization when the outer contact and operating environment change.
The TaOx-based photocathode also maintained a stable photoresponse in the reported tests, including continuous operation in 1 M hydrochloric acid for two hours. The control electrode showed a slight current decrease during testing. These results support the investigation of TaOx for acidic PEC operation, while remaining specific to the tested materials and conditions.
Practical implications for interface engineering
The study demonstrates a thin-film contact strategy that combines silicon passivation with electron transport, using ALD TaOx and a hydrogenation treatment. Its value lies not only in the reported device efficiencies, but also in the linked process insights: interface treatment can change electrical behavior, and thickness optimization requires balancing recombination against contact resistance.
For engineers developing silicon optoelectronic or PEC systems, the practical takeaway is to evaluate the complete contact stack rather than a single layer in isolation. TaOx showed promise in both tested device types, but the optimum configuration depended on film thickness, hydrogenation, and the selected metal or catalyst. Careful interface and process control is therefore central to translating this approach into other device designs.