In ultraviolet nanoimprint lithography (UV-NIL), a thin layer of ultraviolet-curable resin is patterned against a mold and cured with UV light. The process can create nanoscale features, but excess resin often remains between the patterned features and the substrate. This residual layer can complicate subsequent dry etching. Liquid-transfer imprint lithography offers a way to control that layer, although high-viscosity resins make the transfer more challenging. A roll-press approach combined with liquid-transfer imprint lithography was demonstrated to transfer nanoscale patterns while eliminating the residual layer under the reported process conditions.
Why residual layers matter in UV-NIL
During imprinting, resin fills the mold features, but some material may also remain as a continuous film beneath the pattern. This residual layer must be removed before dry etching when the patterned resin is used as an etch mask. A thinner or absent layer is therefore useful for process integration.
Liquid-transfer imprint lithography (LTIL) separates resin distribution from the final imprint. A replica mold is first brought into contact with liquid UV-curable resin on a temporary, or dummy, substrate. When the mold is separated, a thin liquid resin layer remains on its surface. The mold is then brought into contact with the target substrate, where the resin is filled into the pattern and cured.
The method can reduce the amount of resin transferred to the target, but high viscosity makes it harder to form a sufficiently thin, uniform layer. Adding solvent to lower viscosity can introduce another process concern: air bubbles may become trapped in the resin. Roll pressing addresses the challenge mechanically by applying pressure to move excess liquid resin away from the patterned area.
How roll pressing supports liquid-transfer imprint lithography
The reported process used a roller to press the replica mold against the resin-coated substrate. As the roller moved, excess liquid was pushed out of the contact region. The researchers then used parallel-plate UV-NIL to fill the mold pattern and cure the resin. This sequence combined pressure-assisted resin removal with the pattern-filling and curing steps of imprint lithography.
Two UV-curable resins were evaluated: one with a viscosity of 2,900 mPa·s and another with a viscosity of 13,090 mPa·s. Neither could be thinned sufficiently by spin coating alone. The patterns were line-and-space structures with a 1:2 line-to-space ratio, designed at line widths of 990 nm, 540 nm, and 270 nm.
The process also had practical pressure limits. For the 2,900 mPa·s resin, roll pressing was performed at 15.0 MPa. Applying more pressure caused transfer defects. The higher-viscosity resin also required careful pressure control: the roll-press stages were conducted at 15.0 MPa in some steps and 4.0 MPa in another, because higher pressure at those stages could collapse the replica-mold patterns or cause defects.
Different resin viscosities required different transfer sequences
Single transfer sequence for the 2,900 mPa·s resin
With the lower-viscosity of the two tested resins, one LTIL and roll-press procedure produced a pattern with no residual layer. The measured film thickness and pattern height were both 623 nm, which was taken as evidence that the residual layer was zero. A 990 nm line-width pattern was transferred. The line width spread by 18 nm during transfer, which the study attributed to pattern-height collapse.
Repeated processing for the 13,090 mPa·s resin
The higher-viscosity resin did not reach the same result with a single LTIL step. After one transfer, the cured residual layer measured 1.42 μm. The process was therefore modified to repeat roll pressing and liquid transfer before the final imprint on a new silicon substrate. In total, the reported sequence used two LTIL operations and three roll-press operations.
With that repeated sequence, patterns at all three designed line widths—990 nm, 540 nm, and 270 nm—were transferred, and no residual layer was observed for the tested line-and-space structures. As with the lower-viscosity resin, the 990 nm pattern showed an 18 nm line-width spread, attributed to collapse in pattern height.
Process implications for patterning and etching
The results show that the number of transfer and pressing steps can depend on resin viscosity. A single roll-press LTIL sequence was sufficient for the 2,900 mPa·s resin in this experiment, while the 13,090 mPa·s resin required repeated processing. The study also illustrates why pressure cannot simply be increased without limit: excessive pressure led to defects or pattern collapse, depending on the stage and material.
For process engineers evaluating UV-NIL, the practical lesson is to treat resin viscosity, pressure, mold robustness, and transfer sequence as linked variables. A process window that removes excess resin must still preserve the nanoscale features. The reported work used replica molds and specific resins and conditions, so its results do not establish a universal recipe for other materials or equipment.
High-viscosity UV-curable resins can offer properties relevant to dry-etch masks, including high etch selectivity, and may be formulated with different refractive indices. The ability to pattern such materials without a residual layer could therefore be useful where resin functionality matters alongside nanoscale geometry, including potential lab-on-a-chip applications discussed by the authors.
Conclusion
Roll pressing can help liquid-transfer imprint lithography manage excess high-viscosity resin and reduce residual layers in UV-NIL. In the reported trials, the lower-viscosity resin required one LTIL and roll-press sequence, while the higher-viscosity resin needed repeated transfers and pressing to achieve a pattern with no observed residual layer. For industrial process development, the key is balancing resin removal against pressure-related defects and feature collapse, then validating the sequence for the specific resin, mold, and substrate combination.